_Headquarters - English
Argentina - Español
Australia - English
Austria - Deutsch
Belarus - Русский
Belgium - Français
Belgium - Nederlands
Brazil - Brasil-Português
Bulgaria - Български
Canada - English
Canada - Français
China - 中文简体
China(Taiwan) - 中文繁体 (Taiwan)
Colombia - Español
Croatia - Hrvatski
Czech Rep. - Česky
Denmark - Dansk
Finland - suomi
France - Français
Germany - Deutsch
Hungary - Magyar
India - English
Israel - עברית
Italy - Italiano
Japan - 日本語
Mexico - Español
Morocco - Français
Poland - Polski
Portugal - Português
Romania - Română
Russia - Русский
Serbia - Српски
Slovakia - Slovencina
Slovenija - Slovenšcina
South Africa - English
South Korea - 한국어
Spain - Español
Sweden - Svenska
Switzerland - Deutsch
Switzerland - Français
Switzerland - Italiano
Thailand - ไทย
The Netherlands - Nederlands
Turkey - Türk
UAE - English
UK - English
Ukraine - Український
USA - English
Vietnam - Tiếng Việt
ANA SAYFA
HAKKIMIZDA
Genel Bakış
Kurucular
Iscar Türkiye
Araştırma ve Geliştirme
Üretim
Kalite Güvencesi
Küresel Şirket
REACH Küresel Politikası
Çatışma Mineralleri
Etik Kodu
ISCAR Seminars
Bize Ulaşin
ÜRÜN GRUPLARI
Kesme & Kanal Açma
Tornalama
Minyatür
Delik Delme
Frezeleme
Takım Tutucular
Diş Çekme
Mikro Takımlar Bölümü
Kaplama Kaliteleri
Uç Aşınması
Heavy
YAYINLAR
Yeni Ürün Duyurusu
Yayınlar
Broşürler
Referans ve Kullanım Kılavuzları
ISCAR Dünyası Dergileri
LEARNING
ÇEVRİMİÇİ SATIN ALMA
HESAPLAYICI
İşleme Gücü
Kalite İyileştirici
Üretken Geometriler
TECH
KNOW
E-CAT - Electronic Catalog
ITA - ISCAR Tool Advisor
Machining Power
MillThread Advisor
Productive Geometries
Grade Optimizer
IndustRealize
Tech Talk
FAQ
TECH
KNOW
NEW FAQ ADDED
X
/faq.aspx?countryid=20&SearchCatId=2
Groove-Turn & Parting
ISO Turn
Threading
Milling
Hole making
Products Main Page
>
Insert Wear Problems and Solutions
>
Drill Inserts Wear Problems and Solutions
Drilling Inserts Wear Problems and Solutions
SOLID CARBIDE
DRILLING - INDEXABLE HEAD
DRILLING - INDEXABLE INSERTS
Type of Wear
×
Flank Wear
Flank Wear
Cause
High cutting speed
Low wear resistance carbide grade
Remedy
Check that the correct geometry is used
Increase coolant pressure
Change to harder grade
Increase oil concentration percentage
Reduce cutting speed.*** increase feed
×
Crater Wear
Crater Wear
Cause
Excessive cutting temperatures and pressures on the top of the insert
Remedy
Reduce cutting feed
Check that the correct geometry is used
×
Plastic Deformation
Plastic Deformation
Cause
Cutting temperature is too high
Remedy
Check cutting parameters
Reduce cutting feed
Increase coolant pressure/volume
Use harder grade
Check that the correct geometry is used
×
Thermal Cracking
Thermal Cracking
Cause
Excessive variations in surface temperature, intermittent machining, or variations in coolant supply
Remedy
Increase coolant pressure/volume
Increase oll concentration percentage
×
Corner Fracture
Corner Fracture
Cause
Caused by excessive insert wear before indexing the insert
The grade and geometry could be too weak for the applications
Excessive load on the insert
Built-up edge has been formed on the insert
Remedy
Check radial runout
Reduce feed rate increase the speed
Check tool and part clamping rigidity
Check if pocket gripping force is too low, replace the holder
Increase coolant pressure
Improve jet direction in case of external coolant supply
×
Built-up Edge
Built-up Edge
Cause
Cutting zone temperature is too low
Negative cutting geometry
Machining of very sticky materials such as low-carbon steel, stainless steels, and aluminum
Remedy
Increase the feed
Increase cutting speed
Increase coolant pressure
Check oil percentage in the coolant fluid
×
Edge Chipping
Edge Chipping
Cause
Low wear resistance carbide grade
Built-up edge has been formed
Insufficient cutting fluid
Remedy
Reduce feed rate
Increase cutting speed
Increase coolant pressure
Improve jet direction in case of external coolant supply
Change to different geometry
Check tool and part clamping rigidity
×
Chisel Chipping
Chisel Chipping
Cause
Chisel runout is too big
Combine high feed & low speed
Remedy
Reduce feed rate and increase the cutting speed
Check that chisel misalignment does not exceed 0.02mm
Check tool and part clamping rigidity
Check if pocket gripping force is too low, replace the holder
×
Corner Chipping
Corner Chipping
Cause
Radial runout is too big
Insufficient cutting fluid
Remedy
Check radial runout
Reduce feed rate increase the speed
Check tool and part clamping rigidity
Check if pocket gripping force is too low, replace the holder
Increase coolant pressure
Improve jet direction in case of external coolant supply
×
Land Wear
Land Wear
Cause
Cutting speed too high
Low wear resistance carbide grade
Radial runout is too big
Remedy
Check that the correct geometry is used
Check that T.I.R runout does not exceed 0.02mm
Reduce cutting speed
Increase coolant pressure
Improve jet direction in case of external coolant supply
Check and improve tool and part clamping rigidity
Check if pocket gripping force is too low, replace the tool body
×
Flank Wear
Flank Wear
Cause
High cutting speed
Low wear resistance carbide grade
Remedy
Check that the correct geometry is used
Increase coolant pressure
Change to harder grade
Increase oil concentration percentage
Reduce cutting speed.*** increase feed
×
Crater Wear
Crater Wear
Cause
Excessive cutting temperatures and pressures on the top of the insert.
Remedy
Reduce cutting feed
Check that the correct geometry is used
×
Plastic Deformation
Plastic Deformation
Cause
Cutting temperature is too high
Remedy
Check cutting parameters
Reduce cutting feed
Increase coolant pressure/volume
Use harder grade
Check that the correct geometry is used
×
Thermal Cracking
Thermal Cracking
Cause
Excessive variations in surface temperature, intermittent machining, or variations in coolant supply
Remedy
Increase coolant pressure/volume
Increase oll concentration percentage
×
Corner Fracture
Corner Fracture
Cause
Caused by excessive insert wear before indexing the insert
The grade and geometry could be too weak for the applications
Excessive load on the insert
Built-up edge has been formed on the insert
Remedy
Check radial runout
Reduce feed rate increase the speed
Check tool and part clamping rigidity
Check if pocket gripping force is too low, replace the holder
Increase coolant pressure
Improve jet direction in case of external coolant supply
×
Built-up Edge
Built-up Edge
Cause
Cutting zone temperature is too low
Negative cutting geometry
Machining of very sticky materials such as low-carbon steel, stainless steels, and aluminum
Remedy
Increase the feed
Increase cutting speed
Increase coolant pressure
Check oil percentage in the coolant fluid
×
Edge chipping
Edge chipping
Cause
Low wear resistance carbide grade
Built-up edge has been formed
Insufficient cutting fluid
Remedy
Reduce feed rate
Increase the speed
Increase coolant pressure
Improve jet direction in case of external coolant supply
Change to different geometry
Check tool and part clamping rigidity
×
Chisel Chipping
Chisel Chipping
Cause
Chisel runout is too big
Combine high feed & low speed
Remedy
Reduce feed rate and increase the cutting speed
Check that chisel misalignment does not exceed 0.02mm
Check tool and part clamping rigidity
Check if pocket gripping force is too low, replace the holder
×
Land Wear
Land Wear
Cause
Cutting speed too high
Low wear resistance carbide grade
Radial runout is too big
Remedy
Check that the correct geometry is used
Check that T.I.R runout does not exceed 0.02mm
Reduce cutting speed
Increase coolant pressure
Improve jet direction in case of external coolant supply
Check and improve tool and part clamping rigidity
Check if pocket gripping force is too low, replace the tool body
×
Corner Chipping
Corner Chipping
Cause
Radial runout is too big
Insufficient cutting fluid
Remedy
Check radial runout
Reduce feed rate increase the speed
Check tool and part clamping rigidity
Check if pocket gripping force is too low, replace the holder
Increase coolant pressure
Improve jet direction in case of external coolant supply
×
Flank Wear
Flank Wear
Cause
High cutting speed
Low wear resistance carbide grade
Remedy
Reduce cutting speed
Increase coolant pressure/volume
Choose better wear resistance grade
Increase oil concentration percentage
×
Crater Wear
Crater Wear
Cause
Excessive cutting temperatures and pressures on the top of the insert
Remedy
outer insert:
Reduce cutting speed
Choose better wear resistance grade
Change to different chipbreaker
inner insert:
Reduce feed rate
Change to different chipbreaker
×
Plastic Deformation
Plastic Deformation
Cause
Cutting temperature is too high
Remedy
Reduce feed rate
Choose better wear resistance grade
Increase coolant pressure/volume
Choose a different chipbreaker
×
Thermal Cracking
Thermal Cracking
Cause
Excessive variations in surface temperature, intermittent machining, or variations in coolant supply
Remedy
Use tougher grade
Increase coolant pressure/volume
×
Edge Fracture
Edge Fracture
Cause
Caused by excessive insert wear before indexing the insert
The grade and geometry could be too weak for the applications
Excessive load on the insert
Built-up edge has been formed on the insert
Remedy
Use tougher grade
Reduce feed rate
Increase coolant pressure/volume
Change to different chipbreaker
×
Built-up Edge
Built-up Edge
Cause
Cutting zone temperature is too low
Negative cutting geometry
Machining of very sticky materials such as low-carbon steel, stainless steels, and aluminum
Remedy
Increase cutting speed
Change to different chipbreaker
Reduce feed rate
Increase coolant pressure/volume
×
Chipping
Chipping
Cause
Low wear resistance carbide grade
Built-up edge has been formed
Insufficient cutting fluid
Remedy
Choose tougher grade
Reduce feed
Increase coolant pressure/volume
Change to different chipbreaker
×
TECH CENTER
Strengthening Your
Engineering Qualifications
INDUSTREALIZE
Where Ideas
Become a Reality
E - LEARNING
Become an Expert in
the Metal Cutting Industry